Device Fabrication
The key steps of fabricating devices for carbon-based nanoelectronics are:
- Microfabrication (see below)
Microfabrication: Photolithography, Metalization etc.
To learn more about microfabrication processes look at http://en.wikipedia.org/wiki/Photolithography. The most important source of information is always the photoresist manufacture's data sheet (see the T: drive, Group documents\Photoresist documentation). There are also some good textbooks in the OSU library that cover all aspects of microfabrication:
- “Fundamentals of Microfabrication” 2nd Ed. by Madou (excellent level of detail)
- “The science and engineering of microelectronic fabrication” 2nd Ed. by Campbell (good overview)
- “Introduction to microelectronic fabrication” by Jaeger
For some philosophy on how to make a good recipe you might enjoy reading the zen of device making.
Handling clean chips
All experimental physicists working in this field have to learn best practices for handling chips.
Photolithography
Uses chrome masks to expose photoresist. See Photolithography
Mask design
CAD software is used to design and export the patterns needed for photolithography. In some cases you will need to export .dxf files, in other case .gds files. Josh uses AuotoCAD, this is powerful, industry standard software which is free for academic users. Ethan used DesignCAD (2D version) when he worked in Delft. Matt and Landon like to use Layout Editor which is free, open source software.
Chrome masks are patterned using the direct write lithography system on campus. Chrome masks allow us to reach the 2 micron resolution limit of the contact aligner. There are two write lenses (labeled 10 mm and 2 mm), with a 2 µm or 0.5 µm spot size respectively. For the 2 µm spot size, a mask can be exposed at a rate of 1 square inch every 20 minutes regardless of the amount of exposed area. Using the 0.5 um spot size the write time is on the order of 1 square inch every 1.5 hrs. The write times are fairly insensitive to the complexity of the pattern data. However, large arrays of repetitive shapes can take up to 5 times longer to expose than normally expected.
There is an OSU Cleanroom wiki describing operating procedures for the DWL.
| DWL Costs | |
|---|---|
| Laser time | $9/hour |
| Mask blank | $20 |
| developer/etchant/stripper | $26 |
Before the DWL was installed on campus we had to send CAD drawings to a mask making company. Commerically produced chrome masks cost $400 - 800 each.
![]() | Image of a chrome mask made with the DWL 2 µm spot size. The pink is chrome, the grey is transparent. More mask images. |
For less demanding resolution, for example 10-20 micron minimum feature size, a printed transparency can be used. These masks cost about $60 each and are purchased from a company in Bandon. Now we prefer to make chrome masks in the DWL.
Some tips for a successful mask design:
- start with an outline of the size of your substrate/chip. This can help you visualize and efficiently use chip space.
- use text to label your mask (is it a part of a set? use “Mask 1/4”, etc. Also may include your name/lab name, date, the mask name, mask type. For example, “Carly Fengel, Minot Group, 8/2019, FDM Design #2, Graphene Mask, 2/3”)
- minimize the total area occupied by the mask design and text to decrease write time. The mask writer will put a rectangle around the area containing your design and visit each pixel within that rectangle. The smaller this rectangle, the faster the write time (note that the write time is independent of how much of the mask is exposed vs how much is not).
- include alignment marks for masks in a set. Think carefully about the positive and negative space for each layer; you need to be able to see the alignment mark on the chip underneath and the one on the current mask simultaneously.
- if your mask is going to be mostly chrome with only small open regions, consider adding a clear outline a few mm thick around your design. Otherwise you won't be able to see the edges of the chip underneath which will make it difficult to print the design where you want it on the chip.
- if your design is symmetric or on a clear substrate, put an “L” on your mask design large enough to see with the naked eye. This makes it easy to determine the orientation of the chip. I usually include this L on the electrode layer of the mask set so that it gets imprinted in metal on the chip.
- use the metal layer to mark other useful features on the chip design. For example, you can label device sites with coordinates or letters, or use brackets to indicate the location of graphene sites to help create a “target” when transferring graphene to the chip.
- You can make smaller “test” devices on the chip for experimental purposes.
Ebeam lithography
Matt and Ethan have used the ebeam system at CAMCOR (University of Oregon, 50 minute drive). A basic recipe is available.
In September 2011 the new ebeam lithography system was installed in the OSU Electron Microscopy Facility. Doug Kezsler's group, and Inpria are currently the expert users.
Cleaving & Dicing Wafers
The initial photolithography steps are done on 3“ wafers. To grow nanotubes, however, we have to cleave the Si [1 0 0] wafer or ST-cut quartz into smaller pieces that will fit in our furnace. Matt is the expert when it comes to cleaving.
The only way to get truly square quartz pieces is to use a wafer dicing saw. There is one available in the OSU Cleanroom.
Metal deposition
Thermal evaporation
After doing photolithography, a thin layer of metal (tens of nanometers thick) is deposited on a nanotube chip. The interface between nanotube and metal is critical for device operation (for example, we do not store the chip in a gelpak before evaporation. This will lead to hydrocarbon contamination).
Our workhorse deposition system is the thermal evaporator in Janet Tate's lab, 4th floor Weniger Hall. We have used this system for chrome, gold, aluminum, and iron. Please see Matt Leyden for training. Always follow the standard operating procedure in a step by step fashion - missing one step can ruin your sample and the equipment. Matt and Josh renovated this evaporator in summer 2008.
Evaporation boats are made Tungstun and cost $6-8 each (R. D. Mathis). The boats should be kept clean and reused when possible.
Background info about thermal evaporation
Thin film deposition is monitored by a quartz crystal microbalance (QCM). The operator enters the density of the metal, the z-ratio of the metal and the tooling factor of the evaporator. Density and z-ratio can be looked up on a table. The tooling factor is a geometric factor, basically the ratio of the distance between source and QCM and the distance between the source and sample. When the QCM readings do not agree with AFM characterization of film thickness, users typically adjust the tooling factor.
For thermal evaporation, metal is usually held in a boat made out of Tungsten (W) because the melting point of W is 3422 °C. It is possible to break the boat by heating or cooling too fast. It is also bad for the sample if the temperature inside the evaporator gets too hot.
This evaporation table gives useful advice about which metals can be thermally evaporated. Similar information is on the Kurt Lesker website. For example,
- Iron attacks W so thermal evaporation may not be possible.
- Ti outgases when first heated.
- Cr is available in rod form, so a boat is not necessary. Cr is a great sticking layer.
- Pt and Au are both suitable for thermal evporation in a W boat, these metals do not stick well to an oxide surface.
Electron Beam Deposition
The clean room in Kelley has a new ebeam deposition system. Metals like iron & palladium which are difficult to evaporate thermally can be deposited with the ebeam system. Ask Josh Kevek for more information.
Deposition Alternative: Sputtering
Sputtering is an alternative to thermal evaporation that we have not yet explored. The deposition rate should be more stable. Milo Koretski has a beautiful new sputtering system set up in the chemical engineering department which he used for CNT catalyst deposition.
John Wager's group has an ebeam evaporator. E-beam evaporation is especially useful for metals that are hard to control or hard to melt, like iron and molybdenum.
Etching nanotubes
When making devices from aligned CNTs the unused tubes need to be etched. We currently use the O2 plasma in the Owen Hall clean room. This O2 plasma removes photoresist at a rate of about 100 nm/minute. The recipe from Rogers Nature Nanotech 2007 is 50 mTorr, 20 sccm O2, 30 W, 30 s.
More oxygen plasma details.
Vacuum Anneal
See here for the procedure to do this in our e-beam system. Annealing some kinds of nanotube devices in vacuum seems to decrease contact resistance, improve a leaky gate oxide, and remove surface contaminants. Starting in the ~0.01 mTorr range increase the temperature in increments of 100 C. When you get to 600 C, turn off the heater and allow the device to cool in vacuum to ~200 C before venting. So far, results suggest this improves resistances by ~80%. See the Phil Collin's paper for more information.
Cornell Nanofabrication Facility
User fees (March 2010)
- One time fee for introductory training $420
- Daily fee (covers chemical usage) $10
- Mask making $100 for simple, $300 for complex
- Photolithography on the stepper, $60 per hour
- Metal evaporation, $60 per 2 hour session + $0.80 per nm of gold deposited
- Reactive Ion Etching, $30 per hour, need about a 30 minute session to do 500 nm etch.
Other Device Fabrication: Updated January 2017
Overview of GFET Fabrication
(I) On SiO2 substrate (0) -Expose alignment marks on wafer (see: Photolithography Procedures). -Deposit Chromium using E-beam procedures (about 30 nm). -Place sample in PG-remover on hotplate at 65 C to remove photochemicals and excess metal. Leave for about 15 minutes. Using pipette to gently remove as much metal as possible while in solution. Transfer to fresh PG bath on hotplate. Leave overnight. Rinse with IPA and DI water, then dry with N2 to store. (1) Add prepared graphene to chip. (see Preparation of Graphene). Let dry overnight in covered dish. Soak in acetone overnight to remove PMMA. Rinse with IPA and DI water, dry with N2. (2) Spin-coat chip, expose device contacts using photolithography and develop (see: Photolithography Procedures). (3) Dep. Cr or Ti (1 nm) and Au (50 nm) using E-beam. (4) Place sample in PG-remover on hotplate at 60 C to remove photochemicals and excess metal. Leave for about 15 minutes. Using pipette to gently remove as much metal as possible while in solution. Transfer to fresh PG bath on hotplate. Leave overnight. Rinse with IPA and DI water, then dry with N2 to store. (5) Spin-coat chip, expose graphene using photolithography and develop (see: Photolithography Procedures). (6) Plasma-etch to remove excess graphene (see: Plasma Etch Procedures) (7) [optional: to isolate leads] Dep. SiO2 (50-100 nm) everywhere apart from contact regions. Place in PG-remover, following same procedure as for metal deposition.
(II) On glass cover slip (0) [optional: for releasable devices] Use chip with AlO3 already deposited. (1) Add prepared graphene to cover slip. (see: Preparation of Graphene). Let dry overnight in covered dish. Soak in acetone overnight to remove PMMA. Rinse with IPA and DI water, dry with N2. (2) Expose device contacts using lithography and develop (see: Photolithography Procedures). (3) Deposit Cr or Ti (1 nm) and Au (50 nm) using E-beam. (4) Place sample in PG-remover on hotplate at 60 C to remove photochemicals and excess metal. Leave for about 15 minutes. Using pipette to gently remove as much metal as possible while in solution. Transfer to fresh PG bath. Leave overnight. Rinse with IPA and DI water, then dry with N2 to store. (5) Expose graphene using photolithography and develop (see: Photolithography Procedures). (6) Plasma-etch to remove excess graphene (see: Plasma Etch Procedures).
Preparation of Graphene
(1) Cut graphene on copper (Cu) foil to desired size (the side with the graphene on it should be marked). (2) [Oksana’s lab] Spin PMMA (use 2% PMMA in anisole) onto graphene side. a. Turn on air and lights in fume hood; sign in for instrument use. b. Set spin coater to 3000 rpm for 60 s. Use chuck with small holes in top (not o-ring). c. Set Cu sample on chuck, with graphene side facing up, ensuring all holes are covered. Put chuck onto spin coater. d. Open PMMA in fume hood. Cleanly pipette several drops onto graphene. Press “vacuum”; close lid and begin spin coat. e. Carefully remove coated sample and store. (3) [Ethan’s lab] Hard-bake @ 90 C for 60 s. (4) Float in CE200, copper-side down, for about 8 hours. (5) Remove from solution using tongs and plate, and put into water bath (“water PMMA” label) for about 15 minutes. (6) Transfer to fresh DI water bath. Leave for at least 15 minutes (longer is acceptable). Repeat twice more. (7) Store graphene floating in water bath. (now the graphene still has a layer of PMMA on it ⇒ once graphene has dried overnight on substrate, remove PMMA by soaking in acetone overnight, followed with IPA and H2O rinse).
Plasma-etch Procedures
(last edit: 1/2/18 by Carly) (1) Place samples inside chamber. (2) Turn on plama-etcher (switch on back). (3) Press twice (starts power) (4) Toggle left or right to Setup menu, press Use settings: a. Vacuum set point 201.1 b. Atmospheric Vent 00:15 c. Purge Vent 00 d. Gas Stabilize 59 e. Vacuum Alarm 5:00 minutes Important! If the vacuum is not reached by this time limit, system shuts down. f. Plasma Time: 3:00 minutes (5) Press up to return to main menu. Select Commands. Select Plasma to begin process. (6) After timer runs out, go back to Commands menu, and select Off. (7) Remove samples from chamber.
SOP: PC Stamps and Transfers
Before you begin
PC/Chloroform solution should spin on a hot plate at room temperature for at least 4 hours leading up to use. Failure to adequately prepare can make the polymer hard to pipette and cure accurately. In a pinch, 5 minutes in the sonicator may help to reduce this spin time.
Steps 1-4: Making PC Stamps
Steps 5-X: Testing PC Stamps
Steps X-Y: Transfers
1. Making the Stamp
a. clean three glass slides with acetone and IPA. Scratches and dust can be easily identified with the light to the left of the fume hood in room 306, so repeat this step as necessary. Store the cleanest two for later and prepare the third as the scaffold for the stamp.
b. Center a hole punch on a strip of Kapton tape, slightly longer than the width of slide #3, then attach to clean, non-painted side of it. Trim off any excess off the edges.
c. Prepare the tape as usual: remove the hard backing and cut a channel as you would for a PCL stamp, slightly narrower than the hole punch spanning from the hole to the top edge of slide #3.
d. On a fourth (not necessarily cleaned) slide, apply a long piece of Kapton tape over the glass portion, leaving the area coated white clear for grabbing. Remove the backing off the Kapton tape to obtain a poor-quality fly trap.
e. Use scissors to cut a square centimeter of PDMS from a sheet (which should be labeled for PC stamps) and gently apply hard-backing side of the square to the sticky Kapton surface.
f. The applied PDMS has dirty edges and a thin protective film on top. Using a clean razor oriented as close to vertical as possible, cleave two adjacent edges off the PDMS a few mm wide (1). Cut one edge once more, then remove the thin film off it while leaving the PDMS on slide #4 (2) . Lastly, cleave the other edge to produce a cross pattern, leaving a clean square of PDMS with no protective film (3). See the image for a visual representation.
g. Carefully pinching the edges of the small PDMS square with a clean pair of tweezers, place it in the hole-punched center of slide #3. Once complete, your scaffold should look approximately like the following photo. Carefully place it in a slide storage box and continue to preparing the PC.
2. The PC Pull
please read and practice this portion of the process in full before attempting with your carefully prepared materials. Since the PC cures on contact with air, these steps can be particularly prone to error and are time sensitive.
a. On a clean alpha wipe at the edge of the fume hood, place slides #1 and #2 oriented white side up, side-by-side. You should be able to grab the two white grips with one hand in the fume hook and the other outside it. Layer, we will flip the outward-grip side atop the other and, as the title of this section suggests, pull them apart horizontally.
b. Attach a clean, glass pipette from the top drawer to the left of the fume hood to the blue rubber bulb. After removing the lid to the spinning PC, pipette about a quarter of the length of the tube in a line close to the center of the slide with its grip inside the hood.
c. With feet shoulder-width apart facing perpendicular to the fume hood (think riding a skateboard), flip the slide with the outside grip on top of the other and press firmly with two fingers for a couple of seconds. Hinging at the should to keep the forearm level, pull the top slide out of the fume hood, keeping it as level as you can the whole time. When held up to the light in the fume hood, both side should have wide, colorful reflections (Newton rings) caused by the thin film of PC. The bottom slide may have tighter rings and more defects in the film.
d. Store PC slides #1 and #2 in an air-tight container until ready for the next steps.
3. Completing the Stamp
a. Select an area of PC on either slide that is at least as wide as the hole punch. The thin-film interference should change colors over a length on the order of centimeters in this region (indicating uniform thickness) and be free of scratches or dust when held up to a bright light.
b. Hole punch a long strip of Scotch tape and place the hole over the desired region of PC. No bare glass should be visible through the hole, and PC should be cut down to the glass at the outside edges of tape to prevent sticking to the rest of the slide when peeling. Use a wide, flat object such as a piece of PDMS or wafer tons to press the tape down, removing all the bubbles between surfaces while carefully avoiding the exposed PC through the hole in the tape.
c. Using one hand to hold down the two ends of the slide and leveraging the length of the tape, slowly begin peeling up from the slide by one corner, careful not to pull too fast. The PC not attached to the tape should clearly come to a stop under it, and the underside of the tape should be smooth and colorful due to the thin film. If PC failed to adequately adhere to the tape, re-adhere to the slide and press the top again as we did to remove the bubbles.
d. Retrieve the prepared scaffold (slide #3) from storage. Using the leverage of the long scotch tape, peel the PC up from the glass slide and carefully place the hole-punched spot over the PDMS square. If the PC visibly wrinkles upon peeling it up from the slide, throw it away and try again. See the FAQ section at the end for more details.
e. After adhering the PC/Scotch tape to the stamp scaffold (Slide #3), place back on the hot plate for 60ºC for a few minutes to cure.
4. Testing the Stamp
Unlike PCL stamps, the testing step for PC should not permanently alter the shape of the contact surface if done correctly.
a. Place a clean SiO2 chip in the transfer stage, turn on vacuum, and set the temperature to 60ºC. If the stage makes a hissing sound when turning on the vacuum, ensure all three vacuum holes are adequately covered. Slight dust on the chip can be a helpful reference to guage distance.
b. Deploy the PC stamp (mask) over the sample using the button on the bottom left of the control page. One can gauge the separation between the mask and the surface using the measurement labeled “Δ” in the top right of the control page, measured in millimeters.
c. With the safety on (top right of the control page), approach the surface using the z-stage control by eye while looking at the state. At 5X and 10X, it should be safe to approach at max speed until Δ reads 2.5-3mm. This is because unlike the domes used for PCL stamps, the PDMS used for PC stamps is remarkably flat and of a consistent height.
d. The stamp should not make contact above Δ=1.8mm, but a careful stamp operator should reduce the speed as much as possible below 2.5mm. If you are unsure of the separation between the mask and the stage, change the focus and count the layers: there should be clear markings at the PDMS-glass interface (where tape adheres), and the PC-air interface (dust, slight wrinkles, etc.).
e. When you are about to make contact, a faint interference pattern should be visible, through it may appear and produce contact rapidly depending on how flat or tilted the surface of the stamp is. At the lowest possible speed, continue approaching with the z-stage and be careful not to let contact area (should appear yellow) grow too quickly nor too large, as this can ruin the stamp.
f. A good stamp should make contact close to the center where edge defects have the lowest likelihood of tearing the PC. The contact area should expand slowly and controllably when heated in intervals of 2ºC or when using the slowest z-stage speed. You make choose to save microscope images of the various shapes and sizes of the contact area, labelled with temperature or z-separation Δ.
g. Its best to stop contact after you have seen the stamp expand without letting it touch most of the edges with contact. Then slowly pull back and see how the stamp bounces back or if it rips off quickly. It is preferred to have a uniform down movement to backward movement making contact in the same spot it has last contact.
5. Using the Stamp
The largest difference between using and testing the stamp is that instead of a clean SiO2 chip, you will be using a chip with your desired flake. The stamp should be tested at least once within the hours leading up to transfer and preparations should be made for where the stamp is being transferred to, where the chloroform is, and where you will be disposing of waste chloroform. Repeat steps a-d of part 4.
e. If there are large obstructions (dust, other flakes) in the near vicinity (within about 20um) of the flake you desire to transfer, you may want to carefully clean them with a PCL stamp or with an undesirable/unoccupied portion of the PC stamp. Tall objects can distort the otherwise consistent shape and expansion rate of the contact surface leading to folds or tears in the flakes you want to pick up.
f. After pressing the stamp over the desired flake, pickup occurs simply by pulling back, The flake should become transparent or grey as the contact front recedes past where the flake initially began. If the flake is still colorful after pulling back, it was not successfully picked up and you may need to use a higher temperature. Increasing the temperature of the stage can improve adhesion to PC, but it is possible that this further melting can cause melted PC to diffuse over and under the surface of the desired flakes, reducing the cleanliness and efficacy. The following are examples of picked up flakes:
g. If switching chips on the stage is necessary, increase z-separation to above 3mm, return the mask to the loading position, turn off the vacuum, and replace chips. Is it recommended that you first find where you want to transfer to before moving the mask back into operating position.
h. Approaching the surface once again using z-stage control, continue to adjust the position of the mask and stage as necessary. Once Δ measured approximately 2mm, attempt to use the 40X focus, which is calibrated to improve visibility through stamps. After approaching as close as you can without contacting, if you are happy with the positioning of your flake over the substrate, press down hard with the z-stage. if there are few/no bubbles or gaps in the contact area, heat the stage to 200ºC to melt the PC over the substrate.
i. Once heated all the way, you can pull up with the z-stage, leaving your flake trapped between substrate and melted PC. Submerge the chip in a dish of chloroform in the fume hood for 5 minutes. Upon removal of the dish, hold at an angle and let excess fluid evaporate for a moment in the fume hood to avoid rings of residue on the chip.
Common problems (P) and known solutions (S):
P: My completed stamp has large, dark areas around the perimeter of the PDMS.
S: The PDMS likely has overhangs/ underhangs that are changing the way light reflects through the stamp. This can be okay if shaded area is only on one side and you are transferring only one flake, otherwise you should make a new stamp, careful to cut PDMS more vertically.
P: My completed stamp has streaks across the PC-air interface.
S: If streaks are parallel, they likely arise from bending the PC too much while peeling up from the first slide or during transport to the stamp scaffold. The stamp is likely unusable as these creases cause the contact front to expand in short, fast steps rather than smoothly, which can fold your flake.
P: I have a piece of dust on my PC/ between the PDMS and PC/ between the glass and PDMS.
S: The stamp may still be usable for transferring one flake, as long as you use a clean area of the PC surface, In fact, bumps between other layers may slightly improve the PC surface, as PC that is too flat may make contact all at once.
P: My stamp is not lifting off of the surface / is pulling the chip off vacuum!
S: Set the ramping speed to max, turn on the Peltier, and set the stage temperature to 20ºC. Cooling the PC can make it less sticky and shrink it, improving the chances of successful liftoff.
SOP: PCL Stamps
1. Before you begin...
a. PCL should spin on the hot plate at room temperature in room 308 for 24 hours leading up to use. Failure to adequately prepare can make the polymer hard to pipette and cure accurately.
2. Making the Stamp
a. Clean two glass slides with acetone and IPA. Store the cleanest of the two for later and prepare the other as the scaffold for the stamp.
b. Center a hole punch on a strip of Kapton tape, slightly longer than the width of the slide, then attach to clean, non-painted side.
c. Prepare the tape as usual: remove the hard backing of the tape and cut a channel as you would for a PC stamp, slightly narrower than the hole punch spanning from the hole to the top edge of the slide.
d. Select a PDMS dome for the center of the hole on the slide. Ideally this should be much shorter than it is wide, with a smooth circumference and round top.
e. If not yet separated from PDMS film, carefully cut around the dome as close as possible to its edge. Once freed, grab the dome from the sides with tweezers and move to the center of the slide.
f. Once complete, your scaffold should look like the following photo. Carefully place in a slide storage box and continue to prepare PCL
3. Preparing the PCl
a. bring the cleaner prepared slide to the fume hood in 308, place centered on the spinner as depicted below:
b. Once centered, turn on the vacuum line to the left of the e-beam evaporator labelled “spinner.” This secures the slide in place for spinning.
c. Once the cover is locked in place above the slide, turn on the motor module (a red light should come on). ensure that the speed controlled (blue/ black box with green display) is set to 2250 RPM. Hit “ENT” twice to begin spinning.
d. The PCL cures rapidly in air, and a decent amount is required to get sufficient coverage on the slide. Quickly and carefully pipette the PCL over the center of the spinning slide. Condition of the PCL may be hard to gauge while spinning.
e. Press “EXT” on the speed controlled to stop winning. Once halted, turn off the vacuum line and inspect the sample.
f. PCL should be slightly opaque and in a splatter pattern out of the center. If PCL is piled up irregularly, the stamp may come out uneven. If there is a level area larger than the size of the hole punch, continue to finalize the stamp.
4. Completing the Stamp
a. Trim excess PCL from the side of the slide and anneal on the hot plate in room 306 at 90ºC for one minute or until clear. After removing, allow the PCL to cool until once again opaque.
b. Hole punch a long strip of scotch tape and place the hole over the desired region of PCL. No bare glass should be visible through the hole, and PCL should extend at least a couple of mm under the tape in all directions.
c. Trim excess PCL at the outer edges of the scotch tape. Use wafer tongs or other clean, wide surface to adhere the tape to the PCL. PCL is more robust than PC but be careful of accidentally tearing or contacting the PCL in the center hole.
d. Retrieve the prepared scaffold from storage. Using the leverage of the long scotch tape, slowly peel the PCL up from the glass slide and carefully place the hole-punched spot over the PDMS dome.
e. After adhering the PDMS/ Scotch tape to the stripped Kapton tape, place back on the hot plate at 45ºC for one minute.
5. Testing the Stamp
Unlike PC stamps, the testing step for PCL will permanently alter the shape of the contact surface.
a. Place a clean SiO2 chip in the transfer stage, turn on vacuum, and set the temperature to 40ºC. If the stage makes sound when turning on the vacuum, ensure all vacuum holes are adequately covered.
b. With the safety on (top right of the control page), approach the surface by eye while looking at the stage. Since each PDMS dome is different, there is no exact range of z-stage heights at which contact is guarenteed.
c. Once “close” (use your judgement) pivot to the microscope cameras, slow down the speed, and focus through the center of the PDMS dome at the PCL-air interface.
d. When you are about to make contact, a faint interference pattern may be visible. Contact should appear as a small yellow spot.
e. Once contact is made, stop mechanically pressing and heat the stage at 0.6 speed to 65ºC. You may wish to record the z-height delta at which you made contact to reference during use. The image below depicts the expanded PCL (along with a piece of lint)
f. Once the contact area stops expanding or is at desired size, hit “STOP” on the temperature control. As it cools, the contact surface should obtain a grainy texture but remain relatively transparent. Stretch makes in the PCL may extend outwards from the contact region, possibly altering the shape and clarity.
g. Once cooled to room temperature, stamp may release itself. If not, begin to slowly pull the stamp from the surface with the z-stage.
If the contact area is too large, the stamp may tear or pull the chop off the vacuum hole. If this happens, lower the chip back into secured contact and attempt removal again.
h. If liftoff still does not work you may with to cool the stage to 20 ºC using the temperature control. Ensure that the peltier is on and that the ramping speed is set to “MAX”.
6. Tips for Use
a. When cleaning, approach the surface similarly to during testing. The surface should be visible when viewed through the contact region.
b. Do not trust images of flakes seen outside of this window, as they are often distorted by the bent shape of the PDMS dome.
c. Regard the thin, black circumference of the contact region as functional pickup area even through it may not be possible to see through.