- | ==== 1" Furnace growth | + | ==== 1" Furnace growth |
+ | |||
+ | __**Startup/ | ||
+ | |||
+ | - Keep chips ready for growth in furnace | ||
+ | - PNF are for Utah | ||
+ | - PNF - 2 micron trench | ||
+ | - PNR - 2.6 micron trench | ||
+ | - To pressurize: | ||
+ | - Connect hand pump to nipple | ||
+ | - Black button releases pressure | ||
+ | - Pump up to 25 in Hg | ||
+ | |||
+ | Ethanol/ | ||
+ | |||
+ | - Fill out logbook | ||
+ | - Always run purge | ||
+ | - STD growth | ||
+ | - Humidity | ||
+ | - Turn on Dehumidifier | ||
+ | - Humidity should be around 30% | ||
+ | - Check end cap is secure | ||
+ | - Check Ar and H tanks | ||
+ | - 20PSI on both | ||
+ | - Lose around 5psi of argon tank pressure per hour of flowing | ||
+ | - Load in chips. (I have successfully grown 3 at a time, which is all you can fit on the boat. - Dublin) | ||
+ | - Unscrew the end part | ||
+ | - Careful not to drop it | ||
+ | - Attach magnet to end of tray and slide in chip | ||
+ | - Reattach end part | ||
+ | - Current tube 2022: “Tristan” | ||
+ | |||
+ | __**Growth Process**__ | ||
+ | |||
+ | Input purge parameters: | ||
+ | |||
+ | Anneal: | ||
+ | * 30 C | ||
+ | * 3 min | ||
+ | * Hydrogen: 0.45 SLM | ||
+ | * Argon: 1SLM | ||
+ | |||
+ | Transition: | ||
+ | * 0 min (no transition) | ||
+ | |||
+ | Growth: | ||
+ | * 30 C | ||
+ | * 3 min | ||
+ | * Hydrogen 0.45 SLM | ||
+ | * Methanol 0.3 SLM | ||
+ | * Ethanol 0.15 SLM | ||
+ | |||
+ | - Set timer for 5 min and start purge. Will go through anneal and “growth” stages at 30 C | ||
+ | * When changing parameters, give the program a few seconds to get it | ||
+ | * After purge finishes, reinitialize parameters | ||
+ | * Wait until all flow rates show zero | ||
+ | |||
+ | Growth Parameters: | ||
+ | |||
+ | Anneal: | ||
+ | * 800 C | ||
+ | * Hydrogen: 0.45 SLM | ||
+ | * 1 min | ||
+ | |||
+ | Transition: | ||
+ | * 0 min ramp time | ||
+ | |||
+ | Growth: | ||
+ | * 800 C | ||
+ | * 5 min | ||
+ | * Hydrogen 0.45 SLM | ||
+ | * Methanol 0.3 SLM | ||
+ | * Ethanol 0.15 SLM | ||
+ | |||
+ | - Start growth and set a timer for 14:30. When the furnace reaches 798 C, slowly and deliberately slide in tubes | ||
+ | - Once anneal phase begins, set timer for 4:30 min | ||
+ | - To check if it’s working: Ethanol and methanol are bubbling. | ||
+ | - When PID controller clicks off (growth is finished): | ||
+ | - Pull chip to rim of insulating chamber and allow to sit until 790 C | ||
+ | - Pull chip fully out | ||
+ | - When temp is 500 C, open lid | ||
+ | - When temp is 200 C or lower, pull out chip | ||
+ | - The program flows argon before 200C | ||
+ | - Close lid | ||
+ | - Unscrew end connector | ||
+ | - Drag magnet as far to the left as possible | ||
+ | - Grab back end of sled and pull chip straight out | ||
+ | - Grab in center of rod | ||
+ | - Keep the chip level! It’s not connected | ||
+ | - Place chip on beta wipe | ||
+ | - Hold rod while grabbing chip and place chip in holder | ||
+ | - Store rod in quartz tube, cap it up | ||
+ | - Screw end cap back on and seal tube | ||
+ | - Once chamber is cooled back down to room temperature, | ||
+ | |||